Cobalt Based Laser Cladding Powder

Cobalt Based Laser Cladding Powder

Cobalt Base Alloy-Laser Cladding Alloy Powder Introduction of Laser Cladding Co Based Powder: Cobalt base alloys typically contain tungsten and carbon for strengthening. Carbon has low solid solubility in cobalt and therefore, most of it partitions in WC, W2C and M6C or other carbides. These...

Cobalt Base Alloy-Laser Cladding Alloy Powder
Introduction of  Laser Cladding Co Based Powder:
Cobalt base alloys typically contain tungsten and carbon for strengthening. Carbon has low solid solubility in cobalt and therefore, most of it partitions in WC, W2C and M6C or other carbides. These hard phases have a strengthening effect, making such alloys maintain high hardness and strength at temperatures under 800℃. The cobalt-chromium-tungsten-carbon alloys generally have excellent properties to resist high temperature wear, oxidation and thermal fatigue.


Specifications of Laser Cladding Co Based Powder:

Powder

HRC

Chemical Composition

Coating/Overlaying Process  

Mesh Size

C

Cr

Si

B

Fe

Mo

Ni

Co

Mn

W

Co21LA

35

0.30

26.00

0.50

-

1.00

6.00

4.00

Bal

1.00

-

Laser Cladding

100/270 Or 150/300

Co22C

40

0.50

25.00

0.50

-

1.00

12.00

3.50

Bal

1.00

-

Co25

340

0.25

27.00

1.00

-

1.50

5.50

2.80

Bal

0.50

-

CoX-40

35

0.85

24.10

0.30

1.30

1.50

0.40

8.50

Bal

0.50

7.50

Co06

40

1.10

28.50

1.00

2.60

1.50

-

1.50

Bal

0.50

4.40

Co06H

45

1.30

28.50

1.00

0.90

1.50

-

1.50

Bal

0.50

4.40

CoFH

40

1.70

26.00

1.20

-

1.20

-

22.00

Bal

0.50

12.50

Co12

48

1.40

28.50

1.10

-

1.00

-

1.50

Bal

0.50

8.00


Laser Cladding Process Introduction:

Laser Cladding is an alternative to traditional welding and thermal spray. This technology is similar to thermal spray in that it has an energy source to melt the feed stock that is being applied to a substrate. Where it differs is that it uses a concentrated laser beam as the heat source and it melts the substrate that the feed stock is being applied to. This results in a metallurgical bond that has superior bond strength over thermal spray. Additionally the resulting coating is100% dense with no voids or porosity.


Advantages Laser Cladding Process:
One of the advantages of the laser cladding process is the concentrated beam of energy from the laser. It can be focused and concentrated to a very small area and keeps the heat effected zone of the substrate very shallow. This minimizes the chance of cracking, distorting, or changing the metallurgy of the substrate. Additionally the lower total heat minimizes the dilution of the coating with material from the substrate.


Package & Logistics

 Packing: 5 kg packaging in one bottle, 4 bottles in one box

Label: Brand, Neutral or Customized

Delivery: 7- 21 days, by Sea, Air or Express

Four No-Passing Principles for Unqualified Products

No-Passing of Unclear Reasons

No-Passing of Vague Responsibilities 

No-Passing of Unimplemented Education and Treatment 

No-Passing of Unimplemented Corrective and Preventive Action

35.png

FAQ

1.Q. Why choose US?

(1)We have an experienced technical team understanding different applications. So we can give best advice to our customer about choosing materials and process.

(2).For more than 50 years' development,

● Gas atomized system is used for alloy powder production.

● Powder is carefully screened.

● Accurately control the chemical and particle size.

● Product quality is very consistent.

● Customization is accepted.

2.  Q. What is MOQ?
A. No MOQ for our existing stock, for special size, MOQ is 5 KGS.
3. Q. Can I place a mixed order?
A. Sure!
4.Q. Can I get a lower price if I order large quantities?
A. Yes, big order get big discount.
5.Q. Do you provide samples ? Is it free or extra ?
A. Yes, we will send you sample before mass production, and start production by your approval. Most sample is free,  you only need to pay the freight.
6.Q. When you ship my order?
A. Normally 7-18 days after receiving your payment, but it can be negotiated based on order qty and production schedule.
7.Q. If I need any products hurry, could you make them fast for me?
A. Yes. If you are hurry, we will make the products as fast as we can and delivery them in the fast shipment.
8.Q. How can you guarantee the production quality?
A. Our production is based on ISO9001,we have more than 40 years experience of QC team and strictly quality control system in our production process. At the same time, before sent the products, we will send the free sample for you to test.
9.Q. What about the package?
A. It can make as you need and depend on the products shapes. Generally, we can provide iron drum, carton, wooden case, and bag packages.

Cooperative Project:

Joint Tsinghua University to develop Laser Powder and 3D consumable Powder, Joint Shanghai Jiao Tong University and Fudan University to develop alloy amorphous submicron powder material, Joint Harbin Institute of Technology to develop amorphous and submicron powder material, Joint Hebei University of Technology to develop magnetic submicron powder material, Joint Beijin Institute of Technology to develop high temperature alloy submicron powder material, Joint Tianjin University to develop remanufacturing material auto engine, Joint Tianjin University of Technology to develop laser and remanufacturing material, etc. 


Related Products
Inquiry
Local Business Directory, Search Engine Submission & SEO Tools